	China Plastics ›› 2022, Vol. 36 ›› Issue (8): 42-48.DOI: 10.19491/j.issn.1001-9278.2022.08.007
• Materials and Properties • Previous Articles Next Articles
					
													CHEN Baiquan( ), ZHENG Youming, TIAN Jibo, XHANG Lei, WANG Jinsong, LIN Xiajie, DUAN Yapeng
), ZHENG Youming, TIAN Jibo, XHANG Lei, WANG Jinsong, LIN Xiajie, DUAN Yapeng
												  
						
						
						
					
				
Received:2022-04-13
															
							
															
							
															
							
																	Online:2022-08-26
															
							
																	Published:2022-08-22
															
						CLC Number:
CHEN Baiquan, ZHENG Youming, TIAN Jibo, XHANG Lei, WANG Jinsong, LIN Xiajie, DUAN Yapeng. Preparation and properties of polyamide flame⁃retardant composite reinforced with high content of glass fiber[J]. China Plastics, 2022, 36(8): 42-48.
Add to citation manager EndNote|Ris|BibTeX
URL: https://www.plaschina.com.cn/EN/10.19491/j.issn.1001-9278.2022.08.007
| 材料 | 1# | 2# | 3# | 4# | 5# | 6# | 7# | 8# | 9# | 
|---|---|---|---|---|---|---|---|---|---|
| PA6切片 | 32.4 | — | — | 31.9 | — | — | 41.4 | — | — | 
| PA66切片 | - | 32.4 | — | — | 31.9 | — | — | 41.4 | — | 
| PA56切片 | — | — | 32.4 | — | — | 31.9 | — | — | 41.4 | 
| 红磷母粒 | — | — | — | — | — | — | 8 | 8 | 8 | 
| BPS | — | — | — | 13 | 13 | 13 | — | — | — | 
| 三氧化二锑 | — | — | — | 4.5 | 4.5 | 4.5 | — | — | — | 
| 磷氮阻燃剂 | 17 | 17 | 17 | — | — | — | — | — | — | 
| GF | 50 | 50 | 50 | 50 | 50 | 50 | 50 | 50 | 50 | 
| 抗氧剂1098 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 
| 抗氧剂168 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 
| 硬脂酸钙 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 
| 材料 | 1# | 2# | 3# | 4# | 5# | 6# | 7# | 8# | 9# | 
|---|---|---|---|---|---|---|---|---|---|
| PA6切片 | 32.4 | — | — | 31.9 | — | — | 41.4 | — | — | 
| PA66切片 | - | 32.4 | — | — | 31.9 | — | — | 41.4 | — | 
| PA56切片 | — | — | 32.4 | — | — | 31.9 | — | — | 41.4 | 
| 红磷母粒 | — | — | — | — | — | — | 8 | 8 | 8 | 
| BPS | — | — | — | 13 | 13 | 13 | — | — | — | 
| 三氧化二锑 | — | — | — | 4.5 | 4.5 | 4.5 | — | — | — | 
| 磷氮阻燃剂 | 17 | 17 | 17 | — | — | — | — | — | — | 
| GF | 50 | 50 | 50 | 50 | 50 | 50 | 50 | 50 | 50 | 
| 抗氧剂1098 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 
| 抗氧剂168 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 
| 硬脂酸钙 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 0.2 | 
| 项目 | 1# | 2# | 3# | 4# | 5# | 6# | 7# | 8# | 9# | 
|---|---|---|---|---|---|---|---|---|---|
| 密度/g·10 cm-3 | 1.65 | 1.65 | 1.65 | 1.75 | 1.75 | 1.75 | 1.61 | 1.61 | 1.62 | 
| 灰分/% | 50.1 | 50.2 | 49.9 | 50.2 | 50.1 | 50.3 | 49.8 | 49.9 | 50.1 | 
| 拉伸强度/MPa | 169 | 171 | 166 | 194 | 201 | 201 | 184 | 187 | 185 | 
| 弯曲强度/MPa | 262 | 271 | 268 | 291 | 307 | 297 | 298 | 303 | 301 | 
| 弯曲模量/MPa | 15 324 | 15 895 | 15 454 | 15 101 | 15 985 | 15 872 | 15 784 | 15 010 | 15 155 | 
| 缺口冲击强度/kJ·m-2 | 14.1 | 14.2 | 12.6 | 14.8 | 13.2 | 12.5 | 14.2 | 13.1 | 11.2 | 
| 非缺口冲击强度/kJ·m-2 | 56 | 59 | 51 | 63 | 59 | 50 | 56 | 55 | 47 | 
| 热变形温度/℃ | 208 | 244 | 231 | 206 | 248 | 235 | 209 | 245 | 234 | 
| 项目 | 1# | 2# | 3# | 4# | 5# | 6# | 7# | 8# | 9# | 
|---|---|---|---|---|---|---|---|---|---|
| 密度/g·10 cm-3 | 1.65 | 1.65 | 1.65 | 1.75 | 1.75 | 1.75 | 1.61 | 1.61 | 1.62 | 
| 灰分/% | 50.1 | 50.2 | 49.9 | 50.2 | 50.1 | 50.3 | 49.8 | 49.9 | 50.1 | 
| 拉伸强度/MPa | 169 | 171 | 166 | 194 | 201 | 201 | 184 | 187 | 185 | 
| 弯曲强度/MPa | 262 | 271 | 268 | 291 | 307 | 297 | 298 | 303 | 301 | 
| 弯曲模量/MPa | 15 324 | 15 895 | 15 454 | 15 101 | 15 985 | 15 872 | 15 784 | 15 010 | 15 155 | 
| 缺口冲击强度/kJ·m-2 | 14.1 | 14.2 | 12.6 | 14.8 | 13.2 | 12.5 | 14.2 | 13.1 | 11.2 | 
| 非缺口冲击强度/kJ·m-2 | 56 | 59 | 51 | 63 | 59 | 50 | 56 | 55 | 47 | 
| 热变形温度/℃ | 208 | 244 | 231 | 206 | 248 | 235 | 209 | 245 | 234 | 
| 项目 | 1# | 2# | 3# | 4# | 5# | 6# | 7# | 8# | 9# | 
|---|---|---|---|---|---|---|---|---|---|
| 拉伸强度/MPa | 105 | 124 | 101 | 121 | 146 | 123 | 114 | 135 | 113 | 
| 弯曲强度/MPa | 179 | 200 | 184 | 199 | 227 | 205 | 189 | 214 | 201 | 
| 弯曲模量/MPa | 9 912 | 12 222 | 9 887 | 10 101 | 12 292 | 10 461 | 10 557 | 11 542 | 9 988 | 
| 缺口冲击强度/kJ·m-2 | 17.1 | 16.5 | 16.8 | 18.2 | 15.3 | 16.6 | 18.1 | 19.6 | 20.3 | 
| 无缺口冲击强度/kJ·m-2 | 61.2 | 65.2 | 58.5 | 65.1 | 60.3 | 59.1 | 66.5 | 67.3 | 65.4 | 
| 项目 | 1# | 2# | 3# | 4# | 5# | 6# | 7# | 8# | 9# | 
|---|---|---|---|---|---|---|---|---|---|
| 拉伸强度/MPa | 105 | 124 | 101 | 121 | 146 | 123 | 114 | 135 | 113 | 
| 弯曲强度/MPa | 179 | 200 | 184 | 199 | 227 | 205 | 189 | 214 | 201 | 
| 弯曲模量/MPa | 9 912 | 12 222 | 9 887 | 10 101 | 12 292 | 10 461 | 10 557 | 11 542 | 9 988 | 
| 缺口冲击强度/kJ·m-2 | 17.1 | 16.5 | 16.8 | 18.2 | 15.3 | 16.6 | 18.1 | 19.6 | 20.3 | 
| 无缺口冲击强度/kJ·m-2 | 61.2 | 65.2 | 58.5 | 65.1 | 60.3 | 59.1 | 66.5 | 67.3 | 65.4 | 
| 垂直燃烧厚度/mm | 1# | 2# | 3# | 4# | 5# | 6# | 7# | 8# | 9# | |
|---|---|---|---|---|---|---|---|---|---|---|
| 3.2 | 燃烧时间 | 25 | 23 | 20 | 46 | 39 | 33 | 26 | 23 | 19 | 
| 是否滴落 | 否 | 否 | 否 | 否 | 否 | 否 | 否 | 否 | 否 | |
| 阻燃等级 | V⁃0 | V⁃0 | V⁃0 | V⁃0 | V⁃0 | V⁃0 | V⁃0 | V⁃0 | V⁃0 | |
| 1.6 | 燃烧时间 | 57 | 44 | 39 | 55 | 47 | 44 | 39 | 34 | 32 | 
| 是否滴落 | 否 | 否 | 否 | 否 | 否 | 否 | 否 | 否 | 否 | |
| 阻燃等级 | V⁃1 | V⁃0 | V⁃0 | V⁃1 | V⁃0 | V⁃0 | V⁃0 | V⁃0 | V⁃0 | |
| 0.8 | 燃烧时间 | 98 | 84 | 47 | 89 | 86 | 48 | 77 | 75 | 49 | 
| 是否滴落 | 否 | 否 | 否 | 否 | 否 | 否 | 是 | 否 | 否 | |
| 阻燃等级 | V⁃1 | V⁃1 | V⁃0 | V⁃1 | V⁃1 | V⁃0 | V⁃2 | V⁃1 | V⁃0 | |
| 垂直燃烧厚度/mm | 1# | 2# | 3# | 4# | 5# | 6# | 7# | 8# | 9# | |
|---|---|---|---|---|---|---|---|---|---|---|
| 3.2 | 燃烧时间 | 25 | 23 | 20 | 46 | 39 | 33 | 26 | 23 | 19 | 
| 是否滴落 | 否 | 否 | 否 | 否 | 否 | 否 | 否 | 否 | 否 | |
| 阻燃等级 | V⁃0 | V⁃0 | V⁃0 | V⁃0 | V⁃0 | V⁃0 | V⁃0 | V⁃0 | V⁃0 | |
| 1.6 | 燃烧时间 | 57 | 44 | 39 | 55 | 47 | 44 | 39 | 34 | 32 | 
| 是否滴落 | 否 | 否 | 否 | 否 | 否 | 否 | 否 | 否 | 否 | |
| 阻燃等级 | V⁃1 | V⁃0 | V⁃0 | V⁃1 | V⁃0 | V⁃0 | V⁃0 | V⁃0 | V⁃0 | |
| 0.8 | 燃烧时间 | 98 | 84 | 47 | 89 | 86 | 48 | 77 | 75 | 49 | 
| 是否滴落 | 否 | 否 | 否 | 否 | 否 | 否 | 是 | 否 | 否 | |
| 阻燃等级 | V⁃1 | V⁃1 | V⁃0 | V⁃1 | V⁃1 | V⁃0 | V⁃2 | V⁃1 | V⁃0 | |
| 1 | 别明智.高含量玻纤增强尼龙66的制备及性能研究[J].塑料工业,2014,42(12):111⁃114. | 
| BIE M Z. Research on the preparation and property of high content glass fiber reinforced nylon 66[J]. China Plastics Industry, 2014,42 (12): 111⁃114. | |
| 2 | 刘文虎,张利建,刘有才.高流动性尼龙6的玻纤增强改性研究[J].化工技术与开发,2020,49(7):1⁃4. | 
| LIU W H, ZHANG L L, LIU Y C. Glass fiber reinforced modification of high fluidity nylon 6 [J]. Technology and Development Chemical Industry, 2020,49 (7): 1⁃4. | |
| 3 | 陈宜湛,张宇,诸泉 .蒙脱土协效次磷酸盐阻燃剂对玻纤增强尼龙66材料的影响[J].广东化工,2019,46(23):23⁃25. | 
| CHEN Y Z, ZHANG Y, ZHU Q.Synergistic effect of MMT on phosphonic salt flame retarded nylon 66material reinforced by glass fiber[J].Guangdong Chemical Industry,2019,46(23):23⁃25. | |
| 4 | 戴剑,郑一泉,丁超,等.十溴二苯乙烷阻燃尼龙热稳定性改善研究[J].塑料工业,2018,46(8):144⁃149,157. | 
| DAI J, ZHENG Y Q, DING C,et al.Investigation on the thermal stability improvement of decabromodiphenyl ethane flame retardant nylon [J].China Plastics Industry,2018, 46(8):144⁃149,157. | |
| 5 | 付晓婷,李谦,朱凯,等.包覆红磷阻燃增强PA66的性能研究[J].塑料工业,2021,49(9):130⁃133. | 
| FU X T, LI Q, ZHU K, et al. Study on properties of flame retardant reinforced PA66 coated with red phosphorus [J]. China Plastics Industry, 2021,49 (9): 130⁃133. | |
| 6 | 杜晓华, 田际波, 黄志杰. 高性能环保阻燃尼龙的研究进展和发展趋势[C]//全国塑料改性及合金工业技术交流年会暨新材料和项目推介会.杭州:中国工程塑料工业协会, 2011:21⁃22. | 
| 7 | 山西省化工研究所.塑料橡胶加工助剂(第二版)[M].北京:化学工业出版社,2002:365⁃458. | 
| 8 | 李秀峥,李澜鹏,曹长海,等. 生物基尼龙及其单体研究进展[J].工程塑料应用,2018, 46(7): 138⁃141. | 
| LI X Z, LI L P, CAO C H,et al. Research progress of bio⁃based polyamide and its monomer[J]. Engineering Plastics Application,2018,46(7): 138⁃141. | |
| 9 | 福本修. 尼龙树脂手册[M].北京: 中国石化出版社,1994: 3⁃30. | 
| 10 | 吴田田,王学利,俞建勇,等.生物基尼龙56的非等温结晶性能研究[J].纺织导报,2017,5: 98⁃100. | 
| WU T T, WANG X L, YU J Y, et al. Study on non⁃isothermal crystallization kinetics of bio⁃based PA56[J].China Textile Leader, 2017,5: 98⁃100. | |
| 11 | 陈美玉,来悦,孙润军,等. 生物基尼龙56纤维的结晶行为[J]. 纺织学报,2017,12 :7⁃13. | 
| CHEN M Y, LAI Y, SUN R J, et al. Crystallization behavior of bio Based Polyamide56 fiber [J]. Journal of Textile Research, 2017,12 :7⁃13. | |
| 12 | 郭亚飞,郝新敏,李岳玲,等. 生物基尼龙56与尼龙6、尼龙66纤维结构和性能对比研究[C]//中国化纤协会优秀学术论文(上册).天津:中国纺织工程学会,中国化学纤维工业协会,2014: 169⁃174. | 
| 13 | Pieter Gijsman, Rieky Steenbakkers, Christian Fürst, et al. Differences in the flame retardant mechanism of melamine cyanurate in polyamide 6 and polyamide 66[J]. Polymer Degradation and Stability, 2002, 78(2):219⁃224. | 
| 14 | 田际波,郑友明,张磊,等.黑色无卤阻燃尼龙复合材料激光标识性能的研究[J].塑料工业,2020, 48(7): 90⁃94. | 
| TIAN J B, ZHENG Y M, ZHANG L,et al. Study on laser marking properties of black halogen⁃free flame retardant nylon composite[J]. China Plastics Industry,2020, 48(7): 90⁃94. | 
| [1] | JIA Mingyin, DONG Xianwen, WANG Jiaming, CHEN Ke. Effect of impregnation method on vacuum bag press molding process and properties of polyamide 6 composites [J]. China Plastics, 2022, 36(9): 1-6. | 
| [2] | YANG Jin, CHEN Pengran, GAO Peixin. Preparation and flame-retardant mechanism of epoxy foams synergistically modified with DIDOPO and POSS/EG [J]. China Plastics, 2022, 36(9): 38-45. | 
| [3] | SONG Dejian, YU Peng, PENG Jinsong, XU Miaojun. Preparation of flame retardant EVA hot melt adhesive and its application in repairing cables [J]. China Plastics, 2022, 36(9): 53-56. | 
| [4] | MENG Xin, WANG Xiaolong, GONG Weiguang, JIN Yi. Preparation of three⁃sources⁃in⁃one shell⁃core structural flame retardants and its application in poly(lactic acid) [J]. China Plastics, 2022, 36(9): 96-104. | 
| [5] | LI Yafei, SUN Xiaojie, REN Yueqing, ZHANG Yinling. Preparation and properties of flame⁃retarded anti⁃static polyolefin plates [J]. China Plastics, 2022, 36(8): 23-27. | 
| [6] | WU Wei, HU Huanbo, SHEN Hui, ZHAO Tianyu. Dual⁃synergistic effect of 4A zeolite and Ca⁃Mg⁃Al hydrotalcite on intumescent flame retardant PP and its mechanism [J]. China Plastics, 2022, 36(7): 1-7. | 
| [7] | WEI Simiao, SHAO Lushan, XU Zhun, LIU Yanting, ZHAO Siheng, XU Bo. Flame⁃retardant performance of PA6 modified with hypophosphite/siloxane bi⁃functional compound and diethyl aluminum hypophosphite compound [J]. China Plastics, 2022, 36(7): 129-135. | 
| [8] | CHEN Ke, LIU Mingfei, ZHAO Biao, PAN Kai. Research progress in flame retardancy and ablation resistance of silicone⁃modified polymeric materials [J]. China Plastics, 2022, 36(6): 149-154. | 
| [9] | WANG Jinye, TANG Bohu, YANG Lining, XIE Meng, GUO Zechao, YANG Guang. Study on multi⁃jet⁃fusion forming process of PA12 parts [J]. China Plastics, 2022, 36(6): 81-86. | 
| [10] | CHEN Sheng, LIANG Yingchao, WU Fangjuan, FANG Hui, FAN Xinfeng, CHEN Hui, WANG Yonggang. Preparation and interfacial modification of polyamide 6/bidirectional warp⁃knitted glass fiber composites [J]. China Plastics, 2022, 36(5): 24-28. | 
| [11] | LI Mengqi, CHEN Yajun. Research progress in flame⁃retardancy of poly(lactic acid) with nanomaterials [J]. China Plastics, 2022, 36(4): 102-114. | 
| [12] | XU Weihua, ZHENG Yu, SHEN Xiangyang, ZHANG Yan, LIU Juwen, YAN Shijing. Effects of different POSS on properties of phosphorus⁃silicon synergistic flame retardant epoxy resin [J]. China Plastics, 2022, 36(4): 115-120. | 
| [13] | LIU Chuan, XU Miaojun, WANG Jingchun, LI Bin. Effect of expandable graphite on flame retardant performance of vinyl silicone rubber [J]. China Plastics, 2022, 36(4): 15-18. | 
| [14] | XU Rongxia, WEI Gang, WEI Lilan, WU Jiecui, JIANG Yujiang. Friction and wear properties of PE⁃UHMW modified with nano⁃SiO2 and PA6 [J]. China Plastics, 2022, 36(4): 47-52. | 
| [15] | LI Suyuan, LIU Huipeng, GONG Shun, HUANG Guotao, LI Yucai, WU Xin, DENG Jianping, PAN Kai. Preparation and characterization of EVA foaming materials modified with thermoplastic polyamide elastomer [J]. China Plastics, 2022, 36(4): 6-14. | 
| Viewed | ||||||
| Full text |  | |||||
| Abstract |  | |||||